Grout

High slump (8 - 10") concrete. From the Swedish word "groot" which meant porridge.
  • Used to fill cells in hollow units to increase assembly strength and to hold reinforced steel in place.
  • Basic Ingredients:
    • Portland cement - Type I or II.
    • Fine aggregate (sand): maximum size £ 1/4".
    • Coarse aggregate (pea gravel): maximum size £ 3/4".
    • Lime (seldom added).
    • Water: high water / cement ratio to ensure good flowability and complete filling of voids.
    • Admixtures: grout aid - used for high lift, increases fluidity and water retention as well as promoting expansion of grout.
  • Types of Grout:
    • Fine (more commonly used).
    • Coarse.
  • Compressive Strength:
    • Indicator of Q.C.
    • 1992 ACI requires grout compressive strength, (f `g) to at least equal the specific masonry compressive, (f `m), strength and ³ 2000 psi at 28 days.
      • '97 UBC 2103.4.1 only requires that f 'g ³ 2000 psi.
  • Placement:
    • Pore - total height of masonry to be grouted prior to erection of more units.
    • Lift - height of grout placed in a single continuous operation prior to consolidation.
      • Low lift: height is £ 5'
      • High lift: 5' < height £ 24'. Cleanout openings in bottom course at every vertical bar to check grout.
    • Consolidation - eliminate voids and promote flow around reinforcement. For lifts > 12", must use mechanical vibrators.

See Masonry Council for supplemental information on grout.



Send Email to Deb Larson at Debra.Larson@nau.edu


Web site created by the NAU OTLE Faculty Studio
NAUCopyright 1998 Northern Arizona University
ALL RIGHTS RESERVED